A VCI base paper specification sets what the sheet must deliver before your inhibitor goes on: grammage, absorbency, air permeance, pH, water-soluble chloride and sulphate, dry and wet strength, smoothness and moisture, each with a tolerance and a named test method. The base paper has to carry the inhibitor evenly without adding corrosive ions.
Key takeaways
- The base paper carries the inhibitor; it does not protect metal on its own.
- Specify grammage, Cobb, air permeance, pH, chloride, sulphate, dry and wet strength, smoothness and moisture.
- Give every value a tolerance and a named test method, and ask for a COA per lot.
- Fix tolerances after a coating trial on your own line, and test protection on the coated paper.
What does the base paper do in VCI paper?
It is the carrier. The paper holds the inhibitor and releases it: inside a closed pack the inhibitor vaporises, fills the air space and forms a very thin protective film on bare metal, which volatilises again when the pack is opened [1].
For a coating or impregnation line, that mechanism gives the paper three jobs:
- Take up the inhibitor evenly, so every square metre carries a similar load.
- Let the vapour out at the rate the formulation was designed for.
- Add nothing that works against the inhibitor. Water-soluble chloride and sulphate are corrosive ions in contact with metal, which is why base paper specifications cap them. Kaifeng's product page, for example, describes its chloride and sulphate levels as strictly controlled to prevent electrochemical corrosion.
Protection still needs a closed pack and a carrier within about 30 cm of the metal [1], formulations differ by metal, and a 2018 review notes that some VCIs can increase the corrosion rate of non-ferrous metals and alloys [2].
Kaifeng Paper lists its Rustproof Base Paper for VCI converters as a neutral carrier substrate for vapour-phase anti-rust paper, and this guide covers that untreated base paper only. If you buy finished VCI paper for your own parts rather than coating it, see how end users specify finished anti-rust paper.
Coating your own inhibitor?
Send your grammage, reel width, coating method and chemistry limits. We quote rustproof base paper against those limits.
Metal protection papers from Kaifeng
Where is VCI paper made from this base paper used?
Finished VCI paper protects bare metal in packaging, storage and shipping: machined and automotive parts, tools, steel sheet and coils, and other industrial goods. TIS-GDV lists carbon steel, stainless steel, cast iron, galvanized steel, nickel, chromium, aluminium and copper among the metals the VCI method is used for, and says compatibility has to be checked with the manufacturer [1]. In sea-freight packs for steel sheet, VCI paper is one layer of several: TIS-GDV describes a first ply of fibre-reinforced or plastic-coated kraft paper, with a corrosion protection paper such as VCI paper used instead for unoiled cold-rolled sheet, and a PE film of at least 150 µm as the second ply [1].
How long does VCI protection last?
It depends on the formulation, its load, the metal and how well the pack is sealed, so the figure belongs to the finished VCI paper and the pack, not to the base paper. Ask the converter which protection period it has tested and under which storage conditions, and keep the pack closed until use. Once the pack is opened the protective film volatilises, so parts can usually be used straight away [1].
Which properties belong in a VCI base paper specification?
Twelve properties covering format, absorbency and release, chemistry and strength. Give each a target, a tolerance and a test method. Table 1 sets them out with the values on Kaifeng's product page where one is published.
Table 1. VCI base paper properties and why a coating line needs them
| Property | Why it matters on the line | Rustproof Base Paper (product page) |
|---|---|---|
| Grammage | Paper mass carrying the inhibitor load; reel length per tonne | 40–60 g/m² ± 5% |
| Thickness | Reel diameter and wrapping stiffness | 55–85 µm ± 5 |
| Moisture | Curl, dryer load and flatness of the web | 7% (+2) |
| Cobb, upper / wire side | Reference for uptake of water-based coating liquid | 55 ± 10 / 50 ± 10 g/m² |
| Air permeance | How freely vapour leaves the sheet | Not published |
| Smoothness | Evenness of coat weight across the web | Not published |
| pH | Acidity in contact with metal and with the formulation | 6.5–8.0 |
| Water-soluble chloride | Corrosive ion in contact with metal | < 200 ppm |
| Water-soluble sulphate | Corrosive ion in contact with metal | Described as controlled; no figure |
| Tensile MD / CD | Web tension on the coater, slitter and in wrapping | ≥ 3.0–3.5 / ≥ 1.5–2.2 kN/m |
| Wet tensile MD | Strength while the web is wet from coating | ≥ 0.25 kN/m |
| Burst | Resistance to puncture at part edges | ≥ 150–220 kPa |
How should absorbency and air permeance suit your coating method?
Match them to how the inhibitor goes on. An impregnation bath relies on the sheet taking up liquid through its thickness, while a roll or blade coater lays a metered film on the surface. A sheet that absorbs too much wastes formulation and loads the dryer; one that absorbs too little leaves liquid sitting on the surface, where it can dry unevenly.
Cobb is a reference, not a measure of inhibitor load
The Cobb value measures how much water a sheet takes up in a set time. It is useful for matching paper to a water-based formulation, but it does not measure inhibitor uptake, so confirm the load by weighing uncoated and coated samples from a trial. Cobb is usually measured under ISO 535, most often as Cobb60, a 60-second test [3], so ask which method and test time are behind a quoted figure. The two sides of the sheet can differ: Kaifeng's product page gives 55 ± 10 g/m² for the upper side and 50 ± 10 g/m² for the wire side, so state which side faces your applicator.
Air permeance controls release
Once the inhibitor is on the sheet, vapour has to leave the paper to reach the metal. A dense, closed sheet may hold inhibitor back; a very open one may release it faster than the formulation intends. There is no single right figure. Agree a range with your formulator, and name the method and units on the specification.
What chemistry limits should the base paper meet?
A pH window and maximums for water-soluble chloride and sulphate, each tied to a named test method. The paper may sit against bare metal for months.
- pH. ISO 6588-1 covers the pH of aqueous extracts by cold extraction [3]. State which extraction your limit refers to, because results from different methods are not interchangeable. The 2018 review reports that most VCI molecules are most active between pH 5.5 and 8.5 [2]; ask your formulator whether your inhibitor has its own window. Kaifeng's product page lists pH 6.5–8.0.
- Chloride. Name the water-soluble chloride method and its detection limit on the specification. Kaifeng's product page lists chloride below 200 ppm.
- Sulphate. Set a maximum and a method in the same way.
Ask for these results on a certificate of analysis for each lot, with the method and the laboratory named. During qualification, check a few reels yourself or at a third-party laboratory, so you know how the supplier's figures compare with your own.
Which strength, smoothness and moisture values matter on the line?
Dry and wet tensile, burst, surface strength, smoothness and moisture. Together they decide whether the web runs cleanly through coating, drying, slitting and rewinding.
- Dry tensile, MD and CD. Covers web tension on the coater and rewinder, and the wrap's resistance when it is folded round parts.
- Wet tensile. A water-based coating wets the web before the dryer, which is where weak paper breaks. Kaifeng lists wet tensile MD at ≥ 0.25 kN/m.
- Burst. Matters in the end use, where the coated paper is pulled round sharp edges.
- Surface strength. Loose fibres shed on the line end up in the coating and on the customer's parts. Ask for a surface strength or dusting figure and the method behind it.
- Smoothness. Affects how evenly a coater lays down the film. Agree a method and a range.
- Moisture. Affects curl, the dryer load and how flat the web runs. Kaifeng lists 7% (+2). Ask for moisture at delivery and keep reels wrapped until they go on the line.
How should you run a coating trial before fixing the specification?
Run the trial on your own line with your own formulation, then set tolerances from what you measure. The corrosion result belongs to the coated product: a base paper supplier can certify the sheet, but only the coated paper can be tested for protection.
Questions to send with your RFQ
- Which test method and test time stand behind the Cobb value, and on which side?
- Which extraction method stands behind the pH value?
- What are the chloride and sulphate maximums, and which methods and detection limits apply?
- What air permeance and smoothness does the grade reach, by which method?
- What does the certificate of analysis show for each lot?
- Agree a trial sheet with target values and methods for every property in Table 1, and ask for the certificate of analysis for the trial reel.
- Check incoming values for pH, chloride and moisture before the reel goes on the line.
- Run at production speed and coat weight. Record web breaks, curl after drying, dusting at rollers or blades, and wet pick-up.
- Weigh uncoated and coated samples across the web to find the inhibitor load and how much it varies.
- Test the coated paper by the method your customers cite. Research laboratories have used the Eschke test, in which kraft paper dipped in an inhibitor is dried, wrapped round metal coupons and kept in a humidity chamber at 85% relative humidity for 10 days [2].
- Fix the specification from the trial results, with tolerances your line can hold, and repeat a short check on the first production lots.
What should an enquiry for VCI base paper include?
Everything in Table 1 plus your line and delivery details. A supplier who answers each line with figures and methods is easier to qualify than one who sends a brochure.
- Grammage and tolerance, and thickness if your line is sensitive to it
- Application method (impregnation bath, roll or blade coater, size press), formulation type (water- or solvent-based) and line speed
- Cobb target, with the side and method; air permeance range if agreed with your formulator
- pH window and chloride and sulphate maximums, with methods
- Dry and wet tensile, burst and surface strength
- Moisture at delivery
- Reel width, outside diameter, core size, splices allowed per reel and reel wrapping
- What the certificate of analysis must show for each lot
- Annual volume, call-off pattern and delivery destination
Send your base paper specification
Kaifeng Paper supplies rustproof base paper to VCI converters. To compare a grade with your current paper, send your base paper specification sheet for a quote.
- Tell us the grammage, reel width and core.
- Add the coating method, chemistry limits and annual volume.
- We quote rustproof base paper against those limits.
FAQs
What does VCI stand for?
Volatile corrosion inhibitor, sometimes written as vapour corrosion inhibitor. VCI paper is a carrier paper, usually kraft, treated with that inhibitor; the untreated sheet is the base paper this guide covers.
How does VCI paper work?
The paper carries a volatile corrosion inhibitor. Inside a closed pack the inhibitor vaporises, fills the air space and settles on bare metal as a very thin film that keeps moisture off the surface. When the pack is opened the film evaporates, so parts can usually go straight to the next process. The base paper's role is to hold the inhibitor and release it without adding corrosive salts.
What grammage is used for VCI base paper?
There is no single standard grammage. Lighter sheets fold more easily around small parts and give more area per tonne; heavier sheets resist tearing on sharp or heavy parts. Kaifeng's product page lists its rustproof base paper at 40–60 g/m². Choose the grammage with your formulator, because the inhibitor load and its cost are usually worked out per square metre of paper.
Why does chloride in the base paper matter?
The paper may sit against bare metal for months, and water-soluble chloride is a corrosive ion in contact with metal. A base paper with a stated chloride maximum, tested by a named method, removes one variable when a coated product fails a corrosion test.
Can any kraft paper be used as VCI base paper?
Not reliably. Ordinary packaging kraft is usually specified for strength and price, and its data sheet may not list pH, chloride or sulphate. It may still coat well, but without those figures you cannot tell whether a failed corrosion test came from the formulation or from the paper. Ask for a sheet made to a written chemistry specification, with results for each lot.
Is the Cobb value the same as inhibitor uptake?
No. Cobb measures how much water a sheet absorbs in a fixed time under set conditions. It helps compare papers for a water-based formulation, but solvent-based systems behave differently, and inhibitor load also depends on line speed, coat weight and drying. Measure the actual load by weighing uncoated and coated samples taken across the web during a trial.
Who is responsible for corrosion test results?
The converter, or whoever applies the inhibitor. A base paper supplier can certify grammage, strength and chemistry for each lot, but protection depends on the formulation, its load and the pack. Test the coated paper by the method your customers cite, and treat the base paper certificate as one input to that result.
Should VCI base paper be pH neutral?
Usually close to neutral, but the right window comes from your formulation. A 2018 review reports that most VCI molecules are most active between pH 5.5 and 8.5, and Kaifeng's product page lists its base paper at pH 6.5–8.0. Agree the window with your formulator, and name the extraction method on the specification, because results from different methods are not interchangeable.
Compliance note: corrosion protection depends on the VCI formulation, its loading and the packing conditions, and is the responsibility of the party applying the inhibitor. Parameters quoted from Kaifeng's product page are subject to Kaifeng's current specification sheets and test reports.
Sources
- German Insurance Association (GDV), Transport Information Service. "4.4.3 The VCI method (Volatile Corrosion Inhibitor)". TIS-GDV Packaging Handbook, n.d. https://www.tis-gdv.de/tis_e/verpack/verpackungshandbuch/11verpackungshandbuch_0443-htm/ Accessed Nov 2026.
- Ansari F.A., Verma C., Siddiqui Y.S., Ebenso E.E., Quraishi M.A. "Volatile corrosion inhibitors for ferrous and non-ferrous metals and alloys: A review". International Journal of Corrosion and Scale Inhibition 7(2):126–150, 2018. https://doi.org/10.17675/2305-6894-2018-7-2-2 Accessed Nov 2026.
- Cepi-CTS. "Handbook 5:1 List of properties for which samples are provided and their indicative ranges" (Rev. 45). Cepi, 2026. https://www.cepi.org/wp-content/uploads/2026/05/HB51-Properties-list.pdf Accessed Nov 2026.